自放电Self-discharge causes_ BW II.ppt_第1页
自放电Self-discharge causes_ BW II.ppt_第2页
自放电Self-discharge causes_ BW II.ppt_第3页
自放电Self-discharge causes_ BW II.ppt_第4页
自放电Self-discharge causes_ BW II.ppt_第5页
已阅读5页,还剩3页未读, 继续免费阅读

下载本文档

版权说明:本文档由用户提供并上传,收益归属内容提供方,若内容存在侵权,请进行举报或认领

文档简介

1、Causes of self-discharge,Brian Way December 12, 2007,Dendrites caused by metal contamination in cathode This type is responsible for most self-discharging cells Metal dissolves from cathode, plates on anode and grows dendrite through separator See example on next page,Causes of Self-discharge,Exampl

2、e: Fe contamination in cathode,Fe,Anode 1) Fe2+2e- Fe 2) yLixC6 yLix- 2/yC6 + 2Li+2e-,1. Uncharged cell: Fe particle in cathode,3. Self-discharging cell: Fe dendrite grows through separator, touches cathode,Cathode 1) Fe Fe2+2e- 2) yLi1-xCoO2+2Li+2e-yLi1-x+2/yCoO2,2. Charged cell: Fe particle dissol

3、ves And plates on anode,Total reaction: Fe moves from cathode to anode, growing dendrite on anode surface, into separator. Li moves from anode to cathode, discharging cell slightly., e-,Electrons flow from anode to cathode through dendrite, allowing cell to self-discharge. Rate of self-discharge is

4、controlled by resistance of electron path,Facts about metal contamination,Metal must dissolve at cathode potential (4.3V) Fe, Ni, Cu, CuZn (Brass), Steel (most), FeS, many low oxidation state metal compounds Very few metals are stable: Al (passivated), Au, Pt(?), some stainless steels Some materials

5、 take longer than others to form dendrites that conduct Particles must touch the cathode to dissolve Metal contamination in anode does not cause self-discharge Particles must be large enough to form dendrite that penetrates separator Particles diameter should be approx. separator thickness or greate

6、r Self-discharge rate depends on the resistance of the electron path. Cu, Ni, CuZn form better conducting dendrites than stainless steel Cathode is high resistance, so self-discharge is slower if particle is in coated region compared to on bare Al foil,Sources of metal contamination,Raw materials in

7、 cathode Active materials (LiCoO2), Cond. Diluents All processes which may produce metal contamination Especially: Powder handling, slitting, winding, grooving, welding Material may be mixed into cathode, land on cathode surface, or be washed onto cathode edge by wetting process.,How much metal?,One

8、 50um diameter Fe particle= 5x10-7g One cell = 15g LiCoO2 One 50um particle/cell = 5x10-7g/15g = 34ppb Amount of Fe required in 1MT of LiCoO2 to make every cell self-discharge = 34mg,Detecting contaminants in raw material,Very difficult to do because chemical state and size of the metal is important

9、 If metal is substituted in the structure, it may be stable. e.g. LiCo0.99Fe0.01O2 is 100ppm Fe but is OK If particles are small they will not penetrate separator. E.g. Super P has many 10um FeS particles Amount required to cause self-discharge is much smaller than the background amounts in the raw

10、materials Magnetic screening for particles may help find big problems,Other causes of Self-discharge are much less common,Puncture of separator Sharp particle or defect punctures separator Contaminant or defect could be on anode or cathode Can be piece of coating material Hardware shorting Tabs touching can, crimp through gasket Li dendrites Li dendrites can grow through sepa

温馨提示

  • 1. 本站所有资源如无特殊说明,都需要本地电脑安装OFFICE2007和PDF阅读器。图纸软件为CAD,CAXA,PROE,UG,SolidWorks等.压缩文件请下载最新的WinRAR软件解压。
  • 2. 本站的文档不包含任何第三方提供的附件图纸等,如果需要附件,请联系上传者。文件的所有权益归上传用户所有。
  • 3. 本站RAR压缩包中若带图纸,网页内容里面会有图纸预览,若没有图纸预览就没有图纸。
  • 4. 未经权益所有人同意不得将文件中的内容挪作商业或盈利用途。