高压酸浸镍钼矿提取钼和镍_第1页
高压酸浸镍钼矿提取钼和镍_第2页
高压酸浸镍钼矿提取钼和镍_第3页
高压酸浸镍钼矿提取钼和镍_第4页
高压酸浸镍钼矿提取钼和镍_第5页
已阅读5页,还剩13页未读, 继续免费阅读

下载本文档

版权说明:本文档由用户提供并上传,收益归属内容提供方,若内容存在侵权,请进行举报或认领

文档简介

1、高压酸浸镍钼矿提取钼和镍 Trans. Nonferrous Met. Soc. China 232013 3083 ?3088Extraction of molybdenum and nickel from Ni ?Mo ore by pressure acid leaching1,2 1 1 1Si-fu WANG , Chang WEI , Zhi-gan DENG , Cun-xiong LI , 1 1 1 1Xin-bing LI , Jun WU , Ming-shuang WANG , Fan ZHANG1. Faculty of Metallurgical and Energ

2、y Engineering, Kunming University of Science and Technology, Kunming 650093, China; 2. Yunnan Hualian Zinc and Indium Limited by Share Ltd., Wenshan 663701, ChinaReceived 4 September 2012; accepted 26 April 2013Abstract: A direct hydrometallurgical route for nickel and molybdenum extraction from a n

3、ickel ?molybdenum Ni ?Mo ore using pressure acid leaching was studied. The nickel and molybdenum were extracted by acid leaching under oxygen pressure. Compared with traditional roasting methods, this hydrometallurgical method eliminates SO and As O emission the Ni ?Mo ore containing 2 2 315% ?25% S

4、. Compared with existing alkali leaching recovery of molybdenum process, almost all the nickel and considerable molybdenum were extracted in the acid leaching process. Under oxygen pressure conditions, almost all the nickel and a substantial part of the molybdenum were dissolved into the acid leachi

5、ng liquor and the other part of the molybdenum was left in the acid leach residue. The acid leach residue was further leached under alkaline NaOH conditions. Under optimal experimental conditions, the extraction rates nickel and molybdenum reached 97% and 96%, respectivelyKey words: nickel ?molybden

6、um ore; pressure leaching; alkaline leaching; nickel; molybdenum characteristics. Research has therefore been initiated into 1 Introduction treating Ni ?Mo ores by direct metallurgical processes Several processes have been proposed to recover In southern China, the Ni ?Mo ore as a sediment- molybden

7、um from the Ni ?Mo ore, such as roasting, hosted ore layer of the lower Cambrian black shale has NaOH/Na CO leaching under active oxygen conditions 2 3been known to local geologists for at least 40 years 1,2. 6,7, direct leaching with NaOH+Na CO /NaClO 8,9, 2 3 3A partial evaluation of the Ni ?Mo or

8、e deposits and their direct NaOH leaching under active oxygen conditions genesis has been attempted in past decades. In general, 10 and direct leaching with H SO for nickel recovery 2 4the Ni ?Mo ore enriches in nickel, molybdenum and only 11. Moreover, direct bioleaching of molybdenum vanadium and

9、is used for extracting nickel and and nickel from the Ni ?Mo ore has been investigated molybdenum raw materials with a gross reserve of 9.37 using a molybdenum-resistant thermophilic bacterium million tons 1,3. sulfolobus metallicus, but the leaching rate is not very For the Ni ?Mo ore, the classica

10、l process for nickel high and it requires further research 12and molybdenum recovery is roasting, melting and Although an increasing number of articles have concentration to produce a high impurity nickeldealt with the Ni ?Mo ore, few studies report the leaching molybdenum alloy. In the process, sul

11、fur dioxide SO of both molybdenum and nickel by direct metallurgical 2and arsenic trioxide As O release may cause serious processes. In this work, the extraction behavior of nickel 2 3environmental pollution. Mineral processing routes have and molybdenum from the Ni ?Mo ore is studied during been pr

12、oposed for the Ni ?Mo ore 4,5; however, it is the oxygen pressure leaching process, characterized by inefficient to enrich nickel and molybdenum through no sulfuric acid. Various characteristics of the ore-dressing owing to the ores complex mineralogical Ni ?Mo ore are used beneficially and partial

13、sulfur is Foundation item: Projects 51174104, 50874053 supported by the National Natural Science Foundation of China; Project 2009AA06Z106 supported by Hi-Tech Research and Development Program of China; Project 201 supported by Doctoral Fund of Ministry of Education of China Corresponding author: Ch

14、ang WEI; Tel/Fax: +86-871-5188819; weichang502sina DOI: 10.1016/S1003-63261362837-X3084 Si-fu WANG, et al/Trans. Nonferrous Met. Soc. China 232013 3083 ?3088 transformed into sulfuric acid under oxygen pressureLtd and X-ray diffraction XRD, and the pH value of The effects of parameters including lea

15、ching time, the leaching liquor was measured using a PHS-3C digital leaching temperature, liquid-to-solid ratio and initial pH meter from Shanghai Hongyi Instrument Co., Ltdsulfuric acid concentration on leaching efficiency areinvestigated. After oxygen pressure leaching, the acid 3 Results and disc

16、ussion leach residue is further leached by the alkaline solutionfor molybdenum recovery. Optimal time, temperature, 3.1 Characterization of Ni ?Mo ore liquid-to-solid ratio and initial sulfuric acid concentration The compositions of the Ni ?Mo ore are listed in are determined for the extraction of n

17、ickel and Table 1. The XRD pattern of the raw ore shown in Fig. 1 molybdenum to examine the economic viability of the confirms that the Ni ?Mo ore consists of crystalline pyrite, process. quartz, muscovite, millerite and elemental sulfur, butmolybdenum 6.89% was not detected, which occurs 2 Experime

18、ntal mainly in the form of amorphous sulfide MoS and 2co-exists with clay, quartz 13 ?15. Nickel occurs mainly 2.1 Materials as vaesite NiS and millerite NiS 13,16,172The Ni ?Mo ore was collected from GuizhouProvince in China. Analytical grade reagents, including Table 1 Chemical compositions of Ni

19、?Mo ore mass fraction, sulfuric acid, were purchased from Chengdu Union % Institute Chemical & Reagent and commercial pure Mo Ni V Fe S C SiO Al O2 2 3All aqueous solutions were prepared using distilled CaO MgO P F Cu Zn Ti Pb 0.052.2 Experimental procedureThe samples were crushed and ball mille

20、d to 85% 0.074 mm and dried at 75 °C in an oven for 24 hLeaching experiments were conducted at an oxygen partial pressure of 1.2 MPa in an autoclave 1 L titanium alloy cylinder reactor with thermometer and stainless steel tube for injection of industrial oxygen by industrial compressor. The rea

21、ctor was heated with a thermostatically controlled disc-type electric heater and liquid samples were withdrawn during the experimentFor each experiment excluding those that sulfuric acid was added, 400 mL of distilled water and 200 g of sample were poured into the reactor, industrial oxygen was inje

22、cted and the contents were heated to the desiredtemperature under magnetic stirring 500 r/min and Fig. 1 XRD pattern of Ni ?Mo ore well-agitated for the desired reaction time by adiaphragm pump. The acid residue was separated from 3.2 Effect of initial sulfuric acid concentration on the liquid phase

23、 by filtration, washed twice with water, extraction of nickel and molybdenum dried at 75 °C and the nickel and molybdenum contents To investigate the effect of sulfuric acid were analyzedconcentration on the extraction of molybdenum and After oxygen pressure leaching, the acid residue nickel, a

24、 series of experiments were carried out under the was leached under alkaline NaOH conditions in an following conditions: initial H SO concentration of 02 4agitated flask, heated by an electric jacket. The 100 g/L, leaching time of 5 h, leaching temperature of supernatant was filtered and the acid re

25、sidue cake was 150 °C, oxygen partial pressure of 1.2 MPa and liquid- washed twice with water for 20 min, dried at 75 °C and to-solid ratio of 2.0 mL/g. As shown in Fig. 2, over 97% the molybdenum content was analyzedof nickel and 76% of molybdenum were leached whenthe initial sulfuric aci

26、d concentration was 25 g/L. The 2.3 Analytical methods increase in nickel extraction was insignificant and The metal contents of the sample and leaching molybdenum extraction decreased slightly with an residue were determined by atomic absorption increase in initial sulfuric acid concentrationspectr

27、ometry Shanghai Morning Field Equipment Co., Furthermore, sulfuric acid consumption increased andSi-fu WANG, et al/Trans. Nonferrous Met. Soc. China 232013 3083 ?3088 3085more impurities were produced. Compared with the imum extraction of 76% is reached at 5 h. Therefore, experiment that no sulfuric

28、 acid was added, the results to obtain high nickel and molybdenum recoveries, in revealed that the initial sulfuric acid concentration has subsequent experiments, the leaching time was chosen to little impact on the leaching of nickel and molybdenum be 5 hfrom the Ni ?Mo ore. Therefore, water leachi

29、ng of theNi ?Mo ore was optimal under these conditions. 3.4 Effect of leaching temperature on extraction ofnickel and molybdenum The effect of temperature on molybdenum and nickel extraction was investigated from 105 to 165 °C with distilled water, under an oxygen partial pressure of 1.2 MPa, w

30、ithout sulfuric acid and a liquid-to-solid L/S ratio of 2.0 mL/g for 5 h. It can be seen from Fig. 4 that nickel extraction increased with the increase in leaching temperature from 105 to 150 °C. Beyond 155 °C, the extraction rate of nickel increased slowly with an increase in temperature.

31、 Molybdenum extraction rate increased with increasing temperature and increased only slightly beyond 150 °C. Therefore, in subsequent experiments, the leaching temperature was chosen to be150 °C Fig. 2 Effect of initial sulfuric acid concentration on extraction rates of nickel and molybden

32、um3.3 Effect of leaching time on extraction of nickel and molybdenumTo study the role of leaching time on the extraction of molybdenum and nickel, the reaction time was varied between 3 and 9 h. As shown in Fig. 3, the extraction of nickel increases strongly with the increase in leaching time from 3

33、 to 5 h at 150 °C under the condition of a liquid to solid L/S ratio of 2.0 mL/g, without sulfuric acid and oxygen partial pressure of 1.2 MPa. 97% nickel extraction was obtained in 5 h. This is probably becausethe nickel sulfide oxidizes to NiSO , which dissolves 4easily into the acid solution

34、 under such conditions. Fig. 4 Effect of leaching temperature on extraction rates of Therefore, 5 h is sufficient for nickel extraction. While nickel and molybdenum the extraction of molybdenum increases gradually with an increase in leaching time from 3 to 5 h and a 3.5 Effect of liquid-to-solid ra

35、tio on extraction ofnickel and molybdenum The effect of liquid-to-solid ratio on molybdenum and nickel extraction was examined at an oxygen partial pressure of 1.2 MPa, without sulfuric acid and temperature of 150 °C for 5 h. A series of experiments were carried out by varying the liquid-to-sol

36、id ratio in the range of 1.5 ?6.0 mL/g. It can be seen from Fig. 5 that nickel extraction rate decreased slightly from 98% to 96% with increasing liquid-to-solid ratio from 1.5 to 3.0 mL/g and decreased sharply with increase in liquid-to-solid ratio from 3.0 to 6.0 mL/g. Molybdenum extraction rate d

37、ecreased slowly from 76% to 75% with increase in liquid-to-solid ratio from 1.5 to 2.5 mL/g andalso decreased sharply with increase in liquid-to-solid ratio from 3.0 to 6.0 mL/g. The extraction rates of Fig. 3 Effect of leaching time on extraction rates of nickel and molybdenum and nickel decreased

38、sharply with increase molybdenum3086 Si-fu WANG, et al/Trans. Nonferrous Met. Soc. China 232013 3083 ?3088 in liquid-to-solid ratio from 3.0 to 6.0 mL/g. 3.7 Alkaline leaching of acid leach residue Considering various other factors such as agitation After pressure leaching under optimum conditions,

39、and pipe-line delivery in industrial plants, in subsequent based on the fact that the oxidized molybdenum leaches experiments, the leaching liquid to solid L/S ratio was easily under alkaline conditions 7,8, experiments ofchosen to be 2.0 mL/g. alkaline NaOH leaching of the acid leach residue underc

40、onditions close to hydrometallurgical practice also showed good results. The data presented in Table 3 illustrate that nearly 85% Mo extraction can be achieved by alkaline leaching. Coupled with 76% Mo extraction rate in the pressure oxidation leaching process, the total molybdenum extraction rate w

41、as 96% Table 3 Experimental data of alkaline leaching NaOH LiquidTime/ Temperature ExtractionNo. concentration/ solid ratio/h /°C rate/%?1 ?1mol?L mL?g 1 1.0 1 25 3.0 7 2 1.0 2 50 3.0 10 3 1.0 3 75 3.0 114 2.0 3 75 3.0 69 Fig. 5 Effect of liquid-to-solid ratio on extraction rates of 5 2.0 4 75

42、3.0 71 nickel and molybdenum 6 2.5 3 75 3.0 857 2.5 4 75 3.0 85 3.6 Characterization of acid leach residue 8 3.0 3 75 3.0 85 The acid leach residue used in this study composition in Table 2 was obtained after oxygen3.8 Phase changes during oxygen pressure leaching pressure leaching. Almost all nicke

43、l and a substantial XRD analysis was conducted to understand the part of the molybdenum were leached. The X-ray mechanism of pressure leaching. Figure 1 shows the diffraction pattern of the acid leach residue shown in FigXRD pattern of the acid leaching residue, which reveals 6 indicates that the am

44、orphous phase molybdenum that there are four crystalline mineral phases: quartz disulfide MoS in the Ni ?Mo ore changed into 2SiO , anhydrite CaSO , pyrite FeS and MoO ?H Ocrystalline phase MoO ?H O in the pressure leaching 2 4 2 3 23 2Comparing Fig. 6 with Fig. 1 shows that the crystalline process

45、millerite NiS, muscovite CaCO and elemental sulfur 3Table 2 Chemical compositions of acid leach residue mass S phases all disappeared after leaching. The main fraction, % chemical reactions can be expressed by the following equations: Mo Ni V Fe S C SiO Al OMoS s+4.5O g+3H Ol 2 2 2+ 2CaO MgO P Cu Zn

46、 TiO Pb2 MoO ?H Os+4H + 2SO 1 3 2412.46 0.13 1.14 0.044 0.055 0.38 0.24 + 2Ss+H Ol+1.5O g 2H + SO 2 2 24 2+ 2NiSs+2O gNi + SO 3 24+ 2+CaCO s+2H Ca +CO g+H Ol4 3 2 2Based on the previous work 18, the monomeric molybdate ions transform to the molybdenum cations when the leach solution pH is reduced to

47、 less than 1.0Therefore, in the pressure leaching process, the leach liquor pH was 0.5 and the molybdenum dissolution process can be expressed by the following equation:+ 2 +MoO ?H Os+2H MoO +2H Ol 5 3 2 22After pressure leaching, the acid leach residue was alkaline leached for molybdenum recovery,

48、with the chemical reaction expressed by the following equation:? 2MoO ?H Os+2OH MoO +2H Ol 6 Fig. 6 XRD pattern of acid leach residue 3 2 24Si-fu WANG, et al/Trans. Nonferrous Met. Soc. China 232013 3083 ?3088 3087Thus, the leaching process can be summarized as was studied. The optimum parameters we

49、re: without follows: 1 in the oxygen pressure process, oxidation of sulfuric acid, leaching time of 5 h, leaching temperature the sulfide forms sulfuric acid and the molybdenum IV of 150 °C, liquid-to-solid ratio of 2.0 mL/g, oxygen is oxidized to molybdenum VI Eqs. 1 and 2; 2 the partial press

50、ure of 1.2 MPa and stirring rate of 500 r/minincrease in generated sulfuric acid enhances further Under these conditions, the extraction rate of nickel was dissolution of crystalline NiS, MoS , CaCO Eqs. 3, 4 97% and molybdenum 76%. The acid leach residue was 2 3and 5; 3 the molybdenum in the acid l

51、each residue further leached for molybdenum recovery under alkaline further dissolves in the alkaline leach process Eq. 6. conditions and the results indicated that the molybdenumrecovery reached 85% during the leaching process within 3.9 Comprehensive experimental analysis of Ni ?Mo 3 h. Under the

52、condition of 75 °C, atmospheric pressure, ore liquid-to-solid ratio of 3.0 mL/g and NaOH of 2.5 g/L, The Ni ?Mo ore was investigated by single factor, the total extraction rate of molybdenum was 96%. The and then verification experiment was carried out under treatment of the Ni ?Mo ore by oxygen pressure the optimum conditions, and the results are shown in leaching-alkaline leaching process is reasonable and Table 4. At the oxygen pressure acid leaching stage, the feasibleleaching rates of nickel, mol

温馨提示

  • 1. 本站所有资源如无特殊说明,都需要本地电脑安装OFFICE2007和PDF阅读器。图纸软件为CAD,CAXA,PROE,UG,SolidWorks等.压缩文件请下载最新的WinRAR软件解压。
  • 2. 本站的文档不包含任何第三方提供的附件图纸等,如果需要附件,请联系上传者。文件的所有权益归上传用户所有。
  • 3. 本站RAR压缩包中若带图纸,网页内容里面会有图纸预览,若没有图纸预览就没有图纸。
  • 4. 未经权益所有人同意不得将文件中的内容挪作商业或盈利用途。
  • 5. 人人文库网仅提供信息存储空间,仅对用户上传内容的表现方式做保护处理,对用户上传分享的文档内容本身不做任何修改或编辑,并不能对任何下载内容负责。
  • 6. 下载文件中如有侵权或不适当内容,请与我们联系,我们立即纠正。