TX9

CO2焊焊缝熔深报告文件编号:TX9-LS-002零件名称:60%靠背骨架总成零件号:测量人:李革

日期:2015.11.2武汉浦江沿浦汽车零件有限公司正直诚信高效创新C02焊接的检测焊接标准:正直诚信高效创新C02焊接的检测正直诚信高效创新C02焊接的检测1.焊缝1要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.2mm实测熔深:P1=0.93mm,P2=1.28mm实测l料厚:

LP1=0.96mm,LP2=1.15mm正直诚信高效创新C02焊接的检测:2.焊缝2要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.2mm实测熔深:P1=1.03mm,P2=1.22mm实测l料厚:

LP1=0.9mm,LP2=0.65mm正直诚信高效创新C02焊接的检测3.焊缝3要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.2mm实测熔深:P1=0.83mm,P2=0.43mm实测l料厚:

LP1=1.0mm,LP2=1.13mm正直诚信高效创新C02焊接的检测4.焊缝4要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.2mm实测熔深:P1=1.12mm,P2=0.7mm实测l料厚:

LP1=1.02mm,LP2=1.18mm正直诚信高效创新C02焊接的检测5.焊缝5:要求:熔深≥0.2mm;熔宽≥1.07mm;EDL

≥1.07mm。实测熔深:P1=1.69mm,P2=0.81mm实测熔宽:LP1=2.50mm,LP2=4.33mm。实测EDL=4.11mm满足要求正直诚信高效创新C02焊接的检测6.焊缝6:要求:熔深≥0.2mm;熔宽≥1.1mm;EDL

≥1.1mm。实测熔深:P1=1.24mm,P2=1.27mm实测熔宽:LP1=3.59mm,LP2=3.71mm。实测EDL=4.46mm满足要求正直诚信高效创新C02焊接的检测7.焊缝7:要求:熔深≥0.2mm;熔宽≥1.11mm;EDL

≥1.11mm。实测熔深:P1=1.47mm,P2=1.02mm实测熔宽:LP1=2.72mm,LP2=3.08mm。实测EDL=3.23mm满足要求正直诚信高效创新C02焊接的检测8.焊缝8:要求:熔深≥0.2mm;熔宽≥1.09mm;EDL

≥1.09mm。实测熔深:P1=1.33mm,P2=0.84mm实测熔宽:LP1=3.00mm,LP2=4.06mm。实测EDL=3.91mm满足要求正直诚信高效创新C02焊接的检测9焊缝9:要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深:P1=0.91mm,P2=1.20mm实测熔宽:LP1=4.43mm,LP2=5.03mm。实测EDL=6.28mm正直诚信高效创新C02焊接的检测10:焊缝10:要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深:P1=1.51mm,P2=1.67mm实测熔宽:LP1=5.68mm,LP2=6.76mm。实测EDL=12.11mm(满足B13

1540要求)正直诚信高效创新C02焊接的检测11:焊缝11要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=1.09mm,P2=1.89mm实测熔宽

LP1=2.44mm,LP2=4.49mm。实测EDL=4.34mm满足要求正直诚信高效创新C02焊接的检测12:焊缝12要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=1.60mm,P2=1.12mm实测熔宽

LP1=4.12mm,LP2=5.08mm。实测EDL=2.79mm满足要求正直诚信高效创新C02焊接的检测13:焊缝13要求:熔深≥0.2mm;熔宽≥2.5mm;实测熔深P1=1.55mm,P2=0.67mm实测熔宽

LP1=4.71mm,LP2=2.83mm。满足要求正直诚信高效创新C02焊接的检测14.焊缝14要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=1.53mm,P2=0.48mm实测l料厚:

LP1=1.4mm,LP2=0.39mm正直诚信高效创新C02焊接的检测15.焊缝15要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=0.46mm,P2=0.64mm实测l料厚:

LP1=1.05mm,LP2=4.93mm正直诚信高效创新C02焊接的检测16.焊缝16要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=0.79mm,P2=0.66mm实测l料厚:

LP1=1.01mm,LP2=4.92mm正直诚信高效创新C02焊接的检测17.焊缝17要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=0.66mm,P2=0.88mm实测l料厚:

LP1=1.0mm,LP2=4.85mm正直诚信高效创新C02焊接的检测18:焊缝18要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=0.64mm,P2=1.28mm实测熔宽

LP1=2.88mm,LP2=4.95mm。实测EDL=3.78mm满足要求正直诚信高效创新C02焊接的检测19:焊缝19要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=1.53mm,P2=1.33mm实测熔宽

LP1=4.57mm,LP2=3.78mm。实测EDL=5.25mm满足要求正直诚信高效创新C02焊接的检测20

:焊缝20要求熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深P1=1.03mm,P2=0.95mm,实测熔宽LP1=5.66mm,LP2=4.31mm,实测EDL=4.09mm.正直诚信高效创新C02焊接的检测21.焊缝21要求:熔深≥0.2mm;料厚L1=1.0mm;L2=2.5mm实测熔深:P1=0.37mm,P2=0.92mm实测l料厚:

LP1=1.02mm,LP2=2.45mm正直诚信高效创新C02焊接的检测22.焊缝22要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=0.38mm,P2=0.89mm实测l料厚:

LP1=1.02mm,LP2=2.44mm正直诚信高效创新C02焊接的检测23.焊缝23要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=1.02mm,P2=1.12mm实测l料厚:

LP1=0.99mm,LP2=2.41mm正直诚信高效创新C02焊接的检测24:焊缝24要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=0.80mm,P2=1.60mm实测熔宽

LP1=3.91mm,LP2=1.60mm。实测EDL=9.99mm满足要求正直诚信高效创新C02焊接的检测25:焊缝25要求:熔深≥0.2mm;熔宽≥2.0mm;

EDL≥2.0mm。实测熔深P1=1.28mm,P2=0.83mm实测熔宽

LP1=5.17mm,LP2=4.63mm。实测EDL=9.10mm满足要求正直诚信高效创新C02焊接的检测26焊缝26要求:熔深≥0.2mm;熔宽≥2.5mm;

EDL≥2.5mm。实测熔深P1=0.51mm,P2=1.48mm实测熔宽

LP1=4.33mm,LP2=2.75mm。实测EDL=3.62mm满足要求正直诚信高效创新C02焊接的检测27:焊缝27要求:熔深≥0.25mm;熔宽≥2.5mm;EDL≥2.5mm。实测熔深

P1=1.10mm,P2=0.41mm实测熔宽

LP1=4.36mm,LP2=2.71mm。实测EDL=3.14mm满足要求正直诚信高效创新C02焊接的检测28.焊缝28要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.0mm实测熔深:P1=1.1mm,P2=2.0mm实测l料厚:

LP1=0.98mm,LP2=0.96mm正直诚信高效创新C02焊接的检测29.焊缝29要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.0mm实测熔深:P1=0.72mm,P2=2.68mm实测l料厚:

LP1=1.03mm,LP2=0.92mm正直诚信高效创新C02焊接的检测30焊缝30:要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深P1=0.91mm,P1’=0.80mm,P2=0.88mm实测熔宽LP1=3.11mm,LP1’=2.80mm,LP2=5.10mm。实测EDL=2.86mm满足要求正直诚信高效创新C02焊接的检测31.焊缝31要求:熔深≥0.2mm;料厚L1=1.0mm;L2=1.0mm实测熔深:P1=2.0mm,P2=1.1mm实测l料厚:

LP1=0.96mm,LP2=0.98mm正直诚信高效创新C02焊接的检测32:焊缝32:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=0.93mm,P2=1.11mm实测熔宽:LP1=3.61mm,LP2=2.84mm。实测EDL=4.41mm正直诚信高效创新C02焊接的检测33:焊缝33:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=1.36mm,P2=1.30mm实测熔宽:LP1=3.30mm,LP2=4.04mm。实测EDL=7.61mm正直诚信高效创新C02焊接的检测34:焊缝34:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=1.03mm,P2=1.00mm实测熔宽:LP1=4.61mm,LP2=2.92mm。实测EDL=6.18mm正直诚信高效创新C02焊接的检测35焊缝35要求:熔深≥0.25mm;熔宽≥2.5mm;

EDL≥2.5mm。实测熔深P1=0.51mm,P2=1.48mm实测熔宽

LP1=4.33mm,LP2=2.75mm。实测EDL=3.62mm满足要求正直诚信高效创新C02焊接的检测36:焊缝36要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深

P1=1.60mm,P2=1.12mm实测熔宽

LP1=4.12mm,LP2=5.08mm。实测EDL=2.79mm满足要求正直诚信高效创新C02焊接的检测37:焊缝37要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深

P1=1.53mm,P2=1.33mm实测熔宽

LP1=4.57mm,LP2=3.78mm。实测EDL=5.25mm满足要求正直诚信高效创新C02焊接的检测38.焊缝38:要求:熔深≥0.3mm;熔宽≥1.24mm;EDL

≥1.24mm。实测熔深:P1=0.79mm,P2=0.48mm实测熔宽:LP1=3.49mm,LP2=4.17mm。实测EDL=4.48mm满足要求正直诚信高效创新C02焊接的检测39.焊缝39:要求:熔深≥0.3mm;熔宽≥1.18mm;EDL

≥1.18mm。实测熔深:P1=1.81mm,P2=0.69mm实测熔宽:LP1=3.85mm,LP2=3.61mm。实测EDL=3.93mm满足要求正直诚信高效创新C02焊接的检测40.焊缝40:要求:熔深≥0.3mm;熔宽≥1.19mm;EDL

≥1.19mm。实测熔深:P1=1.59mm,P2=0.72mm实测熔宽:LP1=3.49mm,LP2=4.17mm。实测EDL=4.48mm满足要求正直诚信高效创新C02焊接的检测41.焊缝41:要求:熔深≥0.3mm;熔宽≥1.24mm;EDL

≥1.24mm。实测熔深:P1=1.37mm,P2=0.63mm实测熔宽:LP1=2.92mm,LP2=2.97mm。实测EDL=2.88mm满足要求正直诚信高效创新C02焊接的检测42.焊缝42:要求:熔深≥0.3mm;熔宽≥1.19mm;EDL

≥1.19mm。实测熔深:P1=1.55mm,P2=0.51mm实测熔宽:LP1=4.21mm,LP2=3.54mm。实测EDL=3.99mm满足要求正直诚信高效创新C02焊接的检测43.焊缝43:要求:熔深≥0.3mm;熔宽≥1.25mm;EDL

≥1.25mm。实测熔深:P1=1.39mm,P2=0.72mm实测熔宽:LP1=3.82mm,LP2=3.09mm。实测EDL=3.89mm满足要求正直诚信高效创新C02焊接的检测44.焊缝44:要求:熔深≥0.3mm;熔宽≥1.05mm;EDL

≥1.05mm。实测熔深:P1=1.81mm,P2=0.53mm实测熔宽:LP1=3.88mm,LP2=5.20mm。实测EDL=4.34mm满足要求正直诚信高效创新C02焊接的检测45.焊缝45:要求:熔深≥0.3mm;熔宽≥1.01mm;EDL

≥1.01mm。实测熔深:P1=0.87mm,P2=0.51mm实测熔宽:LP1=2.84mm,LP2=2.57mm。实测EDL=4.90mm满足要求正直诚信高效创新C02焊接的检测46.焊缝46:要求:熔深≥0.3mm;熔宽≥1.07mm;EDL

≥1.07mm。实测熔深:P1=1.51mm,P2=1.46mm实测熔宽:LP1=3.21mm,LP2=4.87mm。实测EDL=3.65mm满足要求正直诚信高效创新C02焊接的检测47.焊缝47:要求:熔深≥0.3mm;熔宽≥1.10mm;EDL

≥1.10mm。实测熔深:P1=0.95mm,P2=0.9mmP3=0.58mmP4=0.08mm实测熔宽:LP1=3.25mm,LP2=3.48mmLP3=3.73mmLP4=3.08mm实测

EDL1=3.64mmEDL2=3.55mm满足要求正直诚信高效创新C02焊接的检测48.焊缝48:要求:熔深≥0.3

mm;熔宽≥1.25mm;EDL

≥1.25mm。实测熔深:P1=0.66mm,P2=1.42mm实测熔宽:LP1=3.8mm,LP2=1.9mm。实测

EDL=3.09mm满足要求正直诚信高效创新C02焊接的检测49.焊缝49:要求:熔深≥0.3mm;熔宽≥1.22mm;EDL

≥1.22mm。实测熔深:P1=2.24mm,P2=0.99mm实测熔宽:LP1=4.18mm,LP2=4.47mm。实测EDL=4.73mm满足要求正直诚信高效创新C02焊接的检测50.焊缝50:要求:熔深≥0.3mm;熔宽≥1.24mm;EDL

≥1.24mm。实测熔深:P1=1.35mm,P2=1.52mm实测熔宽:LP1=2.49mm,LP2=3.08mm。实测EDL=3.91mm满足要求正直诚信高效创新C02焊接的检测51.焊缝51:要求:熔深≥0.3mm;熔宽≥1.25mm;EDL

≥1.25mm。实测熔深:P1=1.42mm,P2=0.66mm实测熔宽:LP1=3.80mm,LP2=1.90mm。实测EDL=3.09mm满足要求正直诚信高效创新C02焊接的检测52.焊缝52:要求:熔深≥0.3mm;熔宽≥2.55mm;EDL

≥2.55mm。实测熔深:P1=2.55mm,P2=0.87mm实测熔宽:LP1=3.39mm,LP2=5.91mm。实测EDL=4.77mm满足要求正直诚信高效创新C02焊接的检测53.焊缝53:要求:熔深≥0.3mm;熔宽≥1.2mm;EDL

≥1.2mm。实测熔深:P1=1.33mm,P2=0.65mm实测熔宽:LP1=2.84mm,LP2=3.21mm。实测EDL=3.11mm满足要求正直诚信高效创新C02焊接的检测54.焊缝54:要求:熔深≥0.3mm;熔宽≥1.25mm;EDL

≥1.25mm。实测熔深:P1=1.39mm,P2=0.72mm实测熔宽:LP1=3.82mm,LP2=3.09mm。实测EDL=3.89mm满足要求正直诚信高效创新C02焊接的检测55.焊缝55:要求:熔深≥0.3mm;熔宽≥1.19mm;EDL

≥1.19mm。实测熔深:P1=1.55mm,P2=0.51mm实测熔宽:LP1=4.21mm,LP2=3.54mm。实测EDL=3.99mm满足要求正直诚信高效创新C02焊接的检测56.焊缝56:要求:熔深≥0.3mm;熔宽≥1.24mm;EDL

≥1.24mm。实测熔深:P1=1.37mm,P2=0.63mm实测熔宽:LP1=2.92mm,LP2=2.97mm。实测EDL=2.88mm满足要求正直诚信高效创新C02焊接的检测57:焊缝57:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=0.93mm,P2=1.11mm实测熔宽:LP1=3.61mm,LP2=2.84mm。实测EDL=4.41mm正直诚信高效创新C02焊接的检测58.焊缝58:要求:熔深≥0.3mm;熔宽≥1.18mm;EDL

≥1.18mm。实测熔深:P1=1.81mm,P2=0.69mm实测熔宽:LP1=3.85mm,LP2=3.61mm。实测EDL=3.93mm满足要求正直诚信高效创新C02焊接的检测59.焊缝59要求:熔深≥0.5mm;料厚L1=2.5mm;L2=11mm实测熔深:P1=0.51mm,P2=3.01mm实测l料厚:

LP1=2.46mm,LP2=10.98mm正直诚信高效创新C02焊接的检测60.焊缝60要求:熔深≥0.2mm;料厚L1=1.0mm;L2=2.5mm实测熔深:P1=0.38mm,P2=0.89mm实测l料厚:

LP1=1.02mm,LP2=2.44mm正直诚信高效创新C02焊接的检测61.焊缝61:要求:熔深≥0.3mm;熔宽≥1.24mm;EDL

≥1.24mm。实测熔深:P1=0.79mm,P2=0.48mm实测熔宽:LP1=3.49mm,LP2=4.17mm。实测EDL=4.48mm满足要求正直诚信高效创新C02焊接的检测62.焊缝62:要求:熔深≥0.3mm;熔宽≥1.25mm;EDL

≥1.25mm。实测熔深:P1=1.42mm,P2=0.66mm实测熔宽:LP1=3.80mm,LP2=1.90mm。实测EDL=3.09mm满足要求正直诚信高效创新C02焊接的检测63.焊缝63要求:熔深≥0.2mm;料厚L1=1.0mm;L2=2.5mm实测熔深:P1=0.37mm,P2=0.92mm实测l料厚:

LP1=1.02mm,LP2=2.45mm正直诚信高效创新C02焊接的检测64.焊缝64要求:熔深≥0.2mm;料厚L1=1.0mm;L2=2.5mm实测熔深:P1=1.61mm,P2=0.77mm实测l料厚:

LP1=1.02mm,LP2=2.45mm正直诚信高效创新C02焊接的检测65:焊缝65:要求:熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。实测熔深:P1=1.98mm,P2=1.54mm实测熔宽:LP1=5.69mm,LP2=2.22mm。实测EDL=6.43mm正直诚信高效创新C02焊接的检测66:焊缝66要求熔深≥0.2mm;熔宽≥2.0mm;EDL

≥2.0mm。a≥110°实测熔深

P1=0.87mm,P2=2.17mm,实测熔宽

LP1=4.19mm,LP2=3.32mm,实测EDL=8.29mm

.正直诚信高效创新C02焊接的检测73:焊缝73:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=0.93mm,P2=1.11mm实测熔宽:LP1=3.61mm,LP2=2.84mm。实测EDL=4.41mm正直诚信高效创新C02焊接的检测74:焊缝74:要求:熔深≥0.25mm;熔宽≥2.5mm;EDL

≥2.5mm。实测熔深:P1=1.03mm,P2=1.00mm实测熔宽:LP1=4.61mm,LP2=2.92mm。实测EDL=6.18mm正直诚信高效创新C02焊接的检测75.焊缝75要求:熔深≥0.2mm;料厚L1=1.0mm;L2=5.0mm实测熔深:P1=1.02mm,P2=1.12mm实测l料厚:

LP1=0.99mm,LP2=2.41mm正直诚信高效创新

温馨提示

  • 1. 本站所有资源如无特殊说明,都需要本地电脑安装OFFICE2007和PDF阅读器。图纸软件为CAD,CAXA,PROE,UG,SolidWorks等.压缩文件请下载最新的WinRAR软件解压。
  • 2. 本站的文档不包含任何第三方提供的附件图纸等,如果需要附件,请联系上传者。文件的所有权益归上传用户所有。
  • 3. 本站RAR压缩包中若带图纸,网页内容里面会有图纸预览,若没有图纸预览就没有图纸。
  • 4. 未经权益所有人同意不得将文件中的内容挪作商业或盈利用途。
  • 5. 人人文库网仅提供信息存储空间,仅对用户上传内容的表现方式做保护处理,对用户上传分享的文档内容本身不做任何修改或编辑,并不能对任何下载内容负责。
  • 6. 下载文件中如有侵权或不适当内容,请与我们联系,我们立即纠正。
  • 7. 本站不保证下载资源的准确性、安全性和完整性, 同时也不承担用户因使用这些下载资源对自己和他人造成任何形式的伤害或损失。

最新文档

评论

0/150

提交评论